🌿 BS EN ISO 18134 specifies the determination of the moisture content of solid biofuels by the oven dry method, superseding the former BS EN 14774 series. Moisture is one of the most important quality parameters of solid biofuels (wood chips, sawdust, pellets, briquettes, straw, etc.): it directly affects calorific value, combustion efficiency, storage stability and commercial pricing (wet- or dry-basis weighing), and is a core indicator of biomass supply-chain quality control. BSI implemented the series as an identical adoption of the ISO 18134 International Standards in the EN ISO series, comprising total-moisture determination (reference/arbitration and simplified methods) and moisture in the general analysis sample.
💡 Moisture content is the “basis” for pricing and heat-value conversion of biofuels: moisture fluctuation between batches significantly changes the net calorific value (LHV) and power output. A unified, comparable oven-dry determination underpins contract settlement and boiler-operation adjustment.
1. Series Structure and Scope 📌
| Part | Standard | Subject | Method |
| Part 1 | BS EN ISO 18134-1:2015 | Total moisture — reference (arbitration) method | Drying in an oven at the specified temperature to constant mass; total moisture from the mass loss; reference basis |
| Part 2 | BS EN ISO 18134-2:2017 | Total moisture — simplified method | Simplified procedure (adjusted drying time and sample size) for routine batch QC |
| Part 3 | BS EN ISO 18134-3:2015 | Moisture in general analysis sample | Moisture of the analysis sample ground to the specified particle size, for result-basis conversion of further analyses |
⚠️ Parts 1 (reference) and 2 (simplified) both determine “total moisture” but differ in procedure details: the reference method suits arbitration and higher-accuracy requirements; the simplified method emphasises efficiency and fast turnaround. Results should agree within an acceptable deviation — re-check with the reference method when necessary.
2. Determination Principle and Method 🔬
The principle of the oven dry method: a defined mass of the test portion is dried in an oven at the prescribed temperature to constant mass, and the moisture content is calculated from the mass loss before and after drying. Key steps include:
- Test portion preparation: sample and store per the standard (sealed, moisture-proof), optionally crush to the prescribed particle size for faster drying;
- Weighing: weigh the drying vessel (with lid) and the test portion on a calibrated balance;
- Drying: dry at the prescribed temperature (e.g., 105±2 °C or as specified) and time, cool in a desiccator and reweigh;
- Constant-mass criterion: repeat drying until two successive mass readings meet the requirement;
- Calculation: moisture = (mass before − mass after) / mass before × 100 %, reported as a mass fraction (%).
🚨 Common errors in moisture determination come from moisture absorption and volatilisation: the portion absorbs moisture if exposed to humid air before weighing, and gains mass if cooled without the lid; some volatile matter is also lost at high temperature. All weighing steps must be moisture-controlled and carefully executed.
3. Key Technical Requirements 🛠️
- Sampling and division: follow the relevant sampling standard (e.g., EN ISO 18135) for representativeness; seal to prevent moisture change;
- Drying temperature and time: strictly follow the temperature, time and constant-mass criterion of the part;
- Equipment: oven temperature uniformity, balance accuracy and desiccator condition must meet the requirements;
- Parallel determinations: run the required number of parallels and check repeatability (permissible difference);
- Reporting: state the method (reference/simplified/analysis sample), basis (total/analysis moisture) and parallel results.
✅ Establishing the standardised flow of “sealed sampling — regulated drying — constant-mass check — repeatability verification” in the laboratory stably meets the accuracy requirements of biofuel moisture determination, supporting trade settlement and fuel management.
4. Engineering Practice Applications 🏭
- 🔍 Fuel acceptance and settlement: convert received weight and heat value by moisture (wet/dry basis) as the commercial pricing basis.
- 📐 Boiler/power-plant operation: adjust combustion air and feed rate from fuel moisture to stabilise load and emissions.
- 🔧 Storage and drying management: monitor chip and pellet stockpile moisture for biomass warehousing and turning, preventing heating and spontaneous combustion.
- 📋 Quality system and compliance: with pellet/briquette product standards (e.g., EN ISO 17225), carry out factory inspection to keep products within specification.
5. Frequently Asked Questions ❓
❓ Q: Why are both “total moisture” and “moisture in the analysis sample” specified?
A: Total moisture relates to the feedstock/batch (surface and bound water, directly linked to trade); analysis-sample moisture relates to the ground analytical sample and provides the dry-basis conversion reference for ash, volatile matter, calorific value and other analyses. The purposes differ.
🔍 Q: How to choose between the reference (Part 1) and simplified (Part 2) methods?
A: Use the reference method for arbitration, acceptance and high-accuracy needs; use the simplified method for routine batch QC and fast turnaround. Batch screening may use the simplified method, with the reference method for disputes or critical batches.
🔧 Q: Why does moisture affect the calorific value of biofuels?
A: Water absorbs latent heat of vaporisation during combustion and lowers the combustible fraction, so higher moisture reduces the net calorific value (LHV); boiler efficiency and power output drop, making moisture a key pricing and operating parameter.
📋 Q: How is moisture absorption during weighing avoided?
A: Seal the sample immediately after sampling; after drying, cool briefly and then in a desiccator to room temperature before weighing; keep the vessel covered during weighing to minimise exposure; maintain effective desiccant in the balance and desiccator.
❓ Q: In what units are results reported?
A: Usually as a mass fraction (%, m/m) of wet-basis moisture; give the analysis moisture alongside for dry-basis conversion. State the method, basis and parallel values with their repeatability in the report.