BS EN ISO 14577 — Metallic Materials: Instrumented Indentation Test for Hardness and Materials Parameters

Test method, verification and calibration of testing machines, calibration of reference blocks and coatings
📄 Scanned-version note: Part 4 of this series (BS EN ISO 14577-4:2016) is a scanned document (not machine-readable). This article summarises it from public domain knowledge of the standard’s subject area; the authoritative clauses are those in the BSI published version.

🔬 BS EN ISO 14577 is the British Standard series adopted by BSI from the European standard EN ISO 14577, specifying a method family for determining the hardness and other materials parameters (such as indentation modulus and creep parameters) of metallic materials by instrumented indentation testing. Prepared by ISO/TC 164 (Mechanical testing of metals) together with CEN/TC 459 and entrusted in the UK to Technical Committee ISE/101/5 (Indentation hardness testing), the series is classified under ICS 77.040.10. Unlike conventional hardness tests (Vickers, Brinell) that measure only the residual impression, instrumented indentation continuously records the force-displacement (load-depth) curve during loading and unloading. It therefore yields not only a hardness value but also derived materials parameters such as indentation modulus and the elastic/plastic work ratio, which is particularly valuable for thin films, small specimens and gradient materials.

💡 Instrumented indentation is “micro-region measurement of mechanical properties”: from a single continuous load-depth curve, both hardness and elastic modulus information are obtained in one test, forming the standardised basis of nanoindentation technology.

1. Series Structure and Scope 📌

This batch covers four parts of the series:

Part StandardThemeICSMain Content
BS EN ISO 14577-1:2015Test method77.040.10Principle, apparatus, procedure and result calculation
BS EN ISO 14577-2:2015Verification and calibration of testing machines77.040.10Direct/indirect verification of force and displacement sensors
BS EN ISO 14577-3:2015Calibration of reference blocks77.040.10Calibration of reference blocks and metrological traceability
BS EN ISO 14577-4:2016Test method for metallic and non-metallic coatings (scanned)77.040.10Special requirements for coated/film indentation testing
⚠️ Parts 1–3 primarily address metallic materials; Part 4 extends to metallic and non-metallic coatings (film systems), where the indentation depth is limited by coating thickness and the corresponding depth/thickness ratio requirements apply.

2. Technical Requirements of Each Part 🔧

2.1 Part 1: Test Method

Part 1 specifies the principle and test method of instrumented indentation: an indenter of defined geometry (most commonly the Berkovich three-sided pyramid) is pressed into the specimen surface at a defined loading rate to a preset force or depth, then unloaded in a defined manner, with the load-depth curve recorded continuously. From the curve, parameters such as Martens hardness (HM), indentation hardness (HIT) and indentation modulus (EIT) can be calculated. The part specifies the test force range, test temperature, specimen surface preparation, indentation spacing and result-expression requirements. The 2015 edition supersedes the 2002 edition, with revisions to terminology and calculation details.

2.2 Part 2: Verification and Calibration of Testing Machines

Part 2 specifies the verification and calibration of the instrumented indentation testing machine: including direct calibration of the force application system, the depth measurement system (displacement sensor) and the machine compliance, together with indirect verification using standard hardness blocks, and gives verification intervals and acceptance criteria for each level, ensuring accuracy and traceability of results.

2.3 Part 3: Calibration of Reference Blocks

Part 3 specifies the calibration of standard hardness blocks (reference blocks) used for indirect verification of testing machines: including the block material, uniformity, calibration method, calibration uncertainty and certificate content, so that machine verification can be traced to national or international standards.

2.4 Part 4: Test Method for Coatings

Part 4 addresses metallic and non-metallic coating (film) systems, specifying the special requirements for instrumented indentation testing on coated surfaces: the indentation depth should be controlled so that the substrate does not significantly influence the result (typically of the order of one-tenth of the coating thickness or less), and the effects of surface roughness, residual stress and interface should be considered, in order to evaluate coating hardness and modulus. (Scanned version, compiled from public domain knowledge)

✅ A complete instrumented indentation result carries both hardness and modulus information, and because the curve is recorded continuously it also allows the elastic-plastic behaviour during loading and unloading to be assessed — something conventional hardness testing cannot do.

3. Key Technical Requirements and Test Points 🧪

  • Machine compliance correction: the deformation of the testing machine itself adds to the displacement measurement; it must be determined by calibration and subtracted, otherwise depth and modulus calculations suffer a systematic bias.
  • Indenter condition: the indenter tip shape (area function) directly affects the contact-area calculation; the area function should be periodically verified using a reference specimen.
  • Surface preparation: the specimen surface should be flat and smooth (polished where necessary); surface roughness significantly affects results at small depths.
  • Force and depth control: loading, hold and unloading should follow the prescribed procedure; creep-sensitive materials require control of the hold time.
  • Result expression: reports should state the parameter type (HM/HIT/EIT, etc.), indenter type, test force or maximum depth and environmental conditions.

4. Engineering Practice 🛠️

  • 🔍 Thin film and coating evaluation: micro-region hardness and modulus evaluation of DLC coatings, nitrided layers, chrome plating and similar is a key tool for PVD/CVD process quality control.
  • 🔧 Small and irregular parts: in-situ measurement of small components and cross-sectional gradient materials that are difficult to hold for conventional hardness testing.
  • 📊 Materials development: using indentation modulus and hardness data to establish composition-process-property relationships and screen formulations and heat treatments.
  • 📋 Laboratory capability: establish machine verification and reference-block traceability systems per Parts 2 and 3, meeting ISO/IEC 17025 requirements for equipment and metrological traceability.

5. Frequently Asked Questions ❓

❓ Q: What is the difference between instrumented indentation and conventional hardness testing (for example Vickers)?
A: Conventional methods measure the size of the residual impression after unloading and cannot directly give elastic information; instrumented methods record the load-depth curve continuously and can yield both hardness (for example indentation hardness HIT) and indentation modulus (EIT).
❓ Q: What is the indentation modulus?
A: Indentation modulus (EIT) is an elastic-modulus characterisation value derived from the initial slope of the unloading curve together with the contact area; it bears a defined relation to the true elastic modulus and is used to compare the elastic behaviour of materials.
❓ Q: Why is machine compliance calibration essential?
A: Under load, the machine frame deforms elastically, adding to the displacement measurement. If not subtracted, the depth is overestimated and the modulus underestimated. Part 2 gives a method for directly determining compliance.
❓ Q: What does Part 4 apply to?
A: It applies to metallic and non-metallic coating (film) systems, such as hard coatings and functional films; the indentation depth must be controlled relative to coating thickness to avoid substrate influence.
🔒
正在加载下载地址,请稍候 10 秒

Leave a Reply

Your email address will not be published. Required fields are marked *