BS EN 15384 — Porosity of Flexible Aluminium Tube Internal Coating Test Series

Packaging — Test Method to Determine the Porosity of the Internal Coating of Flexible Aluminium Tubes (2017 Edition)

🧴 The BS EN 15384 series is the European standard for test methods to determine the porosity of the internal coating of flexible aluminium tubes (e.g., toothpaste, cosmetic and ointment tubes), adopted by the British Standards Institution (BSI) as BS EN 15384-1:2017 and BS EN 15384-2:2017. It specifies two methods — the sodium chloride test and the copper sulphate test — to evaluate the protective capability of the internal coating on the aluminium substrate, providing the basis for packaging quality control and product shelf-life assurance.

💡 The internal coating of a flexible aluminium tube isolates the contents from the aluminium substrate, preventing contents from corroding the tube, aluminium ions from contaminating the contents, and the coating itself from being attacked. Porosity reflects coating integrity and density, directly affecting product stability and shelf life, so BS EN 15384 is widely used in packaging quality control.

1. Series Structure and Scope 📌

The BS EN 15384 series consists of two parts, using two different electrochemical/chemical indicator methods:

PartTest MethodPrincipleApplicability
BS EN 15384-1:2017Sodium chloride testElectrochemical indication of pores via a sodium chloride electrolyteGeneral internal-coating porosity measurement
BS EN 15384-2:2017Copper sulphate testChemical deposition of copper to indicate poresRapid visual indication of pore locations

UK participation was entrusted to Subcommittee PKW/0/-/10 (Packaging — Plastics) of Technical Committee PKW/0 (Packaging), and the series is classified under ICS 55.120 (Packaging containers). The two parts together supersede BS EN 15384:2007.

⚠️ The two methods rely on different indicator principles and differ in sensitivity and applicability. The sodium chloride test detects pores electrochemically (quantitatively/semi-quantitatively); the copper sulphate test reveals pore locations visually by deposition. Choose the method according to quality requirements and product characteristics.

2. Principle of the Methods 🔬

Both methods use electrochemical or chemical reactions between the aluminium substrate and the coating to indicate pores (pinholes, cracks and other defects) in the coating:

  • Sodium chloride test (Part 1): the internally coated tube is placed in a sodium chloride solution; solution reaching the aluminium through pores causes electrochemical action (e.g., corrosion current or hydrogen evolution) indicating the presence and extent of pores. The method is sensitive to fine pores and gives quantitative or semi-quantitative evaluation.
  • Copper sulphate test (Part 2): the tube is placed in a copper sulphate solution; solution reaching the aluminium through pores triggers a displacement reaction depositing copper on the aluminium, forming visible spots that directly reveal pore locations and counts.

The two methods reveal coating defects through different physical-chemical phenomena and complement each other, together giving a comprehensive porosity evaluation.

3. Apparatus and Reagents ⚗️

The standard specifies requirements for apparatus and reagents:

  • Test solutions: sodium chloride or copper sulphate solutions of specified concentration and purity.
  • Test container: a container able to hold the specimen and solution without interfering with the test.
  • Electrodes and measuring apparatus (Part 1): electrodes and instruments for applying/measuring electrochemical parameters.
  • Timing device: to control immersion/energising time.
  • Observation and measurement tools: for observing and quantifying deposits or electrochemical response.

Reagent purity and concentration directly affect results; use the specified grade and prepare solutions strictly per the standard.

4. Test Procedure 📏

The procedure for both methods is broadly similar:

  • Prepare and clean the aluminium tube specimen by the specified method, ensuring the surface is free of contamination and extrinsic defects.
  • Immerse the specimen in the specified solution and soak or energise for the specified time and temperature.
  • For the copper sulphate test, observe and count the copper spots on the tube; for the sodium chloride test, measure the electrochemical response.
  • Assess coating porosity from the observations or measurements and compare with the specified acceptance criterion.
🚨 Specimen preparation and cleaning are critical to accuracy. Residual grease, dirt or scratches cause artefacts and misjudgement of porosity. Clean the specimen strictly per the standard before testing and avoid damaging the coating.

5. Expression of Results 📊

Results are usually expressed as the number of pores per unit area or per unit tube length (e.g., spots per cm²) or as electrochemical response parameters. The standard requires the test report to include:

  • Identification, dimensions and coating type of the tube;
  • The test method used (Part 1 or Part 2);
  • Solution concentration, temperature and test time;
  • Observed or measured results;
  • Conclusion compared with the acceptance criterion.

Porosity is the core quality indicator of the internal coating, directly governing the protection of the contents and the product shelf life.

6. Engineering Practice and Application 🛠️

  • 🔍 Incoming and finished-product inspection: tube manufacturers and fillers should test the porosity of internally coated tubes to control coating quality.
  • 🔧 Coating-process optimisation: use porosity tests to evaluate the effect of coating parameters (e.g., oven temperature, coating thickness, curing time) on coating density.
  • 📊 Product stability assessment: high-porosity tubes allow contents to react with the aluminium substrate, affecting stability and shelf life; assess via testing.
  • 📋 Supplier management: when purchasing tubes, verify the supplier’s porosity test reports and quality system to ensure stable coating quality.

7. Frequently Asked Questions ❓

❓ Q: What is the difference between BS EN 15384-1 and 15384-2?
A: Part 1 uses the sodium chloride test (electrochemical), sensitive to fine pores; Part 2 uses the copper sulphate test (chemical displacement), visually showing pore locations. They differ in principle and can be used complementarily.
❓ Q: Why is internal-coating porosity important?
A: Porosity reflects coating integrity and density. Many pores let contents reach the aluminium, causing corrosion, aluminium-ion migration, product deterioration and reduced shelf life.
❓ Q: Why does the copper sulphate test produce copper spots?
A: Copper sulphate solution reaching the aluminium through pores displaces copper ions which deposit as metallic copper, forming visible spots at the pores, thus directly indicating pore locations and numbers.
❓ Q: How does this series relate to BS EN 15384:2007?
A: BS EN 15384-1:2017 and BS EN 15384-2:2017 together supersede BS EN 15384:2007, splitting the original single method into two parts and detailing the sodium chloride and copper sulphate methods separately.
❓ Q: Why must the specimen be cleaned before testing?
A: Surface grease, dirt or scratches cause artefacts, affecting pore indication and judgement. The standard requires strict cleaning and avoidance of damage to ensure accurate results.
🔒