🏗️ BS EN ISO 17660 specifies requirements for welding of reinforcing steel used in concrete, and is the international standard for controlling reinforcing steel weld quality in construction. The series consists of two parts: Part 1 specifies requirements for load-bearing (structural) welded joints, while Part 2 specifies requirements for non load-bearing (non-structural) welded joints. The UK standards BS EN ISO 17660-1:2006 and BS EN ISO 17660-2:2006 are identical implementations of EN ISO 17660-1:2006 and EN ISO 17660-2:2006, prepared by BSI Technical Committee WEE/43 (Welding of steel for concrete reinforcement), replacing the withdrawn BS 7123.
Reinforcing steel welding is widely used in reinforced concrete structures for splicing bars, fixing intersection points (welded mesh), anchorage, and prefabricated element connections. Load-bearing joints transmit structural loads and require high weld strength and ductility; non load-bearing joints (such as welded mesh intersections) mainly provide positioning and construction functions, with relatively lower requirements. Weld quality directly affects structural safety, so systematic process requirements and inspection methods are essential.
The series consists of two parts, both classified under ICS 25.160.10 (Welding processes). They were developed by ISO/TC 44 (Welding and allied processes), converted to European standards by CEN/TC 121 (Welding), and adopted as British Standards by BSI. They should be used in conjunction with the BS EN 1011 series (welding process recommendations) and national annexes.
| Standard | Title | Published | Joint Type |
|---|---|---|---|
| BS EN ISO 17660-1:2006 | Welding — Welding of reinforcing steel — Part 1: Load-bearing welded joints | Sep 2006 | Load-bearing (structural) joints |
| BS EN ISO 17660-2:2006 | Welding — Welding of reinforcing steel — Part 2: Non load-bearing welded joints | Sep 2006 | Non load-bearing (non-structural) joints |
Load-bearing welded joints transmit axial load in the bars. Common forms include flash butt welding, pressure gas welding, arc welding (lap, groove, and plate welding), and mechanical connections. The standard specifies welding process, weld dimensions, quality requirements, and inspection acceptance for load-bearing joints, and requires welding procedure qualification to verify joint strength and ductility through tensile and bending tests.
Key requirements for load-bearing joints include equal-strength matching of weld and base metal, conformity of weld dimensions (e.g., plate length, weld thickness), the structure and properties of the heat-affected zone, and the static and fatigue performance of the joint. The standard sets allowable limits for weld defects (porosity, slag, cracks, undercut).
Non load-bearing welded joints are mainly used for fixing intersection points of welded mesh and bar cages, and for positioning and construction connections that do not directly transmit primary structural loads. The standard specifies welding process and quality requirements, focusing on the firmness and consistency of intersection welds to prevent loosening during transport, concreting, and vibration.
Requirements for non load-bearing joints are relatively relaxed, but weld quality consistency must still be ensured to prevent false or detached welds. The standard specifies inspection methods such as visual inspection, hammer testing, or destructive testing to verify the reliability of intersection welds.
| Comparison | Part 1 (Load-bearing) | Part 2 (Non load-bearing) |
|---|---|---|
| Functional role | Transmit structural loads | Positioning, construction connection |
| Strength requirement | Equal strength, higher | Relatively lower |
| Procedure qualification | Required (tensile/bending) | Necessary (consistency verification) |
| Inspection focus | Weld dimensions, defects, strength | Weld firmness, consistency |
The standard sets explicit quality requirements for reinforcing steel welded joints, including weld appearance (no cracks, no slag, no severe undercut), weld dimension deviations, and the mechanical properties of load-bearing joints (tensile strength, bending performance). Inspection methods include visual inspection, dimensional measurement, tensile testing, bend testing, and metallographic examination.
Load-bearing joints should be sampled for inspection, and full inspection performed where necessary; non load-bearing joints may use visual and hammer inspection. The standard specifies inspection lots, sample sizes, and acceptance criteria, and requires defective joints to be repaired or scrapped.