BS EN 60754 — Test on Gases Evolved During Combustion of Materials from Cables Standard Series

Determination of Halogen Acid Gas Content and Determination of Acidity (pH) and Conductivity (IEC 60754 Series)

🔥 BS EN 60754 is the British Standards Institution series adopting European Standard EN 60754, identical to IEC 60754, which specifies test methods for gases evolved during combustion of materials from cables (including insulation and sheath). The series characterises the toxic/acidic gas release of halogen-containing cable materials under fire conditions. Part 1 covers the determination of the halogen acid gas content; Part 2 covers the determination of acidity (by pH measurement) and conductivity. The series was prepared by Technical Committee GEL/20/18, Electric Cables — Fire testing, and together with BS EN 60754-1/-2 supersedes the earlier BS EN 50267 series.

🚨 Hydrogen halide gases (such as hydrogen chloride, HCl) released when cable materials burn are acidic and corrosive to equipment and harmful to personnel, representing a major secondary hazard in fires. Low-halogen or halogen-free cables reduce this corrosive impact by controlling halogen acid gas content and acidity, so this series is a key basis for selecting and qualifying fire-resistant cables.

1. Scope and General Framework 📌

The BS EN 60754 series is identical to IEC 60754, prepared by IEC/TC 20 “Electric cables”, and was adopted in the UK by Subcommittee GEL/20/18, Electric Cables — Fire testing, of Technical Committee GEL/20. The 2014 editions of Part 1 (including the IEC corrigendum of November 2013) and Part 2 jointly supersede BS EN 50267-1, 50267-2-1, 50267-2-2 and 50267-2-3 (1999 editions). The series specifies the apparatus, methods and result expression for sampling and determining gases produced from cable material samples (insulation, sheath, filler) under controlled combustion, for assessing the acidic and corrosive gas release characteristics of materials in fire.

⚠️ The series measures the gas-production characteristics of “materials” under standard combustion conditions, not the actual gas release of a complete cable in a real fire. Selection and assessment should consider the overall cable structure, dose and burning conditions, and refer to the limits in relevant product standards.

2. Structure of the Series 📋

Standard NumberTitleIEC ReferenceMain Content
BS EN 60754-1:2014Test on gases evolved during combustion of materials from cables — Part 1: Determination of the halogen acid gas contentIEC 60754-1:2011 + corrigendum Nov. 2013Collect combustion gases in an absorption solution and determine hydrogen halide (acid gas) content
BS EN 60754-2:2014Test on gases evolved during combustion of materials from cables — Part 2: Determination of acidity (by pH measurement) and conductivityIEC 60754-2:2011Absorb combustion gases in water and determine the pH and conductivity of the solution

3. Key Technical Requirements 🔧

3.1 Determination of Halogen Acid Gas Content (Part 1)

Part 1 specifies the method for determining halogen acid gas content: a sample of cable material of known mass is combusted in a tube furnace at a specified temperature (e.g. 800 ℃), the evolved gases are collected in an absorption solution (such as water or alkali), and the halide ions (mainly chlorine, bromine, fluorine) are determined by chemical analysis (e.g. titration or ion-selective electrode), expressed as a percentage of the sample mass. This method assesses the halogen level of the material and is the basis for halogen-free judgement and limit compliance.

3.2 Determination of Acidity and Conductivity (Part 2)

Part 2 specifies the method for determining acidity and conductivity: the combustion gases are led into deionised water for absorption, and the pH and conductivity of the solution are measured. pH reflects the acidity of the solution (the more acidic, the lower the pH), while conductivity reflects the total ion content. These two parameters assess the corrosivity of the combustion gases to the environment and are important indices for evaluating low-acidity cable materials.

Test ItemMeasured ParameterTest PointsEvaluation Significance
Halogen acid gas contentHalide ion mass percentageTube furnace combustion, absorption collection, chemical analysisHalogen level and halogen-free judgement basis
Acidity determinationAbsorption solution pHAbsorb combustion gases in water, measure pHDegree of gas acidity/corrosivity
Conductivity determinationAbsorption solution conductivityAbsorb combustion gases in water, measure conductivityTotal ion content in the solution

3.3 Apparatus and Result Expression

The series specifies the requirements for the tube furnace, combustion tube, absorption bottles, gas-flow control and connecting tubing, and specifies the sample preparation, combustion temperature, gas flow and absorption solution as test conditions, together with the method for calculating and expressing results. Tests should be performed in repeat conditions and reported in a specified manner to ensure comparability between laboratories.

4. Engineering Practice and Application 🛠️

  • 🔍 Selection of low-halogen/halogen-free cables: in places with high personnel density and sensitive electronic equipment (e.g. metros, hospitals, data centres, control rooms), prefer low-halogen or halogen-free cables, using the BS EN 60754 measurement results to judge whether materials meet halogen acid gas and acidity limits.
  • 🔧 Cable design and formulation development: material suppliers use the series to evaluate the gas-release characteristics of insulation and sheath formulations, adjusting formulations (e.g. using halogen-free flame retardants) to reduce halogen content and acidity to meet product standard requirements.
  • 📊 Fire-safety assessment: include halogen acid gas content, acidity and conductivity results in the fire-risk assessment of buildings and industrial facilities, selecting cable routing and protection measures reasonably to reduce secondary corrosion hazards in fire.
  • 📋 Quality conformance inspection: incorporate the series into the quality conformance inspection plan for cable materials and finished cables, periodically sampling to verify that the low-halogen/halogen-free performance of batches remains stable.
✅ Determining the halogen acid content, acidity and conductivity of gases evolved from cable materials in accordance with BS EN 60754 is an important part of quality evaluation and fire-safety design for low-halogen/halogen-free cables, and should be combined with product-standard limits for selection and inspection.

5. Frequently Asked Questions ❓

❓ Q: What is the difference between BS EN 60754-1 and BS EN 60754-2?
A: Part 1 determines halogen acid gas content, typically by chemical analysis of halide ion mass percentage, directly reflecting halogen level; Part 2 absorbs the combustion gases in water and measures pH and conductivity, reflecting the overall acidity and corrosivity of the gases. The two assess the corrosive hazard of combustion gases from different angles.
❓ Q: Why is halogen acid gas a significant hazard in fire?
A: Halogen-containing materials (e.g. PVC) release hydrogen halide gases such as hydrogen chloride on combustion; these form acids in water, corroding metal equipment and structures and irritating the respiratory tract, making escape more difficult. Low-halogen/halogen-free materials significantly reduce this secondary hazard.
❓ Q: Do halogen-free materials necessarily meet acidity limits?
A: Not necessarily. Halogen-free mainly addresses halogen content, but combustion gases may still contain other acidic components (such as sulphur and nitrogen oxides). Therefore, besides halogen acid content, pH and conductivity must be determined per Part 2, and other toxicity and corrosivity tests may be needed.
🔍 Q: How does this series relate to BS EN 50267?
A: BS EN 60754-1/-2 (2014) supersede and integrate the earlier BS EN 50267 series (50267-1, 50267-2-1/-2/-3), unifying halogen acid gas content and acidity/conductivity determination under the IEC 60754 framework, consistent with international methods.
🔒